Troble Shooting

Chalky

Problem / Question
After glazing there is not enough translucency.

Cause (1)
The High Temp is too low.
Solution / Answer (1)
Adjust the high temp so that the surface is slightly shiny after the first bake.
Cause (2)
The Low Temp is too high.
Solution / Answer (2)
Strictly follow the recommended Baking Program.
Cause (3)
Other manufacturer's forming liquid was used.
Solution / Answer (3)
Use Noritake forming liquid. Other manufacturer's forming liquids have too much organic components.
Cause (4)
The vacuum pump is not working properly.
Solution / Answer (4)
Repair the pump if 72mm (28.4 in) vacuum level is not reached in less than 60 seconds.
Cause (5)
Dirty cleaning solution is contaminating the porcelain surface.
Solution / Answer (5)
Use fresh solution in the ultrasonic cleaner.
Cause (6)
Wet porcelain was applied on top of excessively dry porcelain - preventing complete fusion of the porcelain.
Solution / Answer (6)
Be more careful about moisture control especially during prolonged build-ups.